Why Seals Pass Inspection but Fail on Cool-Down
Release time:2026-11-18

The retort lid leaked at 121 °C. Seal strength, peel force and tray flange were all in spec. The leak appeared on cool-down, not in the cook — that timing is the diagnostic clue.
At filling, a bead of sauce crosses the flange and the bar seals straight over it. At 121 °C the fat softens, and the pressure cycle pushes steam along the seal until it finds the edge. On cooling, the channel is already there.
Conventional leak testing reveals only a moistened tray, as the evidence is dissipated within the retort cycle. The failure is visible only at the instant of sealing — a stage generally outside in-line monitoring.
In our internal testing, peelable PP film reads 3.6–3.9 N/15 mm (upper bar 130 °C, lower bar 80 °C) and peels cleanly after a 121 °C, 30-minute retort. These are internal reference values only. Selection should be validated against tray substrate, fill weight and process parameters. When evaluating suppliers, request the full verification chain: sealing conditions, post-retort peel, and behavior on a contaminated flange.
When did you last watch a lid get sealed with sauce on the flange?
Contact Hubei Jinde Packaging if you need technical support.
Previous page
Contact Us
Contact: Ms Zhang
E-mail: scarlette@jindepack.com
Add: Changxing Road No.2, Xiaonan Economic Development Zone, Xiaogan City,Hubei, China